4.2 Weathering Resistance W(s) (Surface Method)

This test is carried out by placing freshly polished glass plates in a chamber at +50°C, 85% humidity for 24 hours. If the glass surface is severely attacked, another 6 hours test is carried out with new test pieces. A classification into four groups is then undertaken by inspecting the treated surface through a 50x microscope as per table 5.

Group Classification
1 When there is no fading on the glass exposed in the chamber for 24 hours - inspected at 6000 luxes
2 When there is no fading observed on the glass exposed in the chamber for 24 hours at 1500 luxes but fading is observed at 6000 luxes
3 When fading is observed on the glass exposed in the chamber for 24 hours - inspected at 1500 luxes
4 When fading is observed on the glass exposed in the chamber for 6 hours - inspected at 1500 luxes