Thermal Properties |
Strain Point (°C) |
StP |
533 |
Annealing Point (°C) |
AP |
562 |
Transformation Temperature (°C) |
Tg |
580 |
Yield Point (°C) |
At |
622 |
Softening Point (°C) |
SP |
700 |
Expansion Coefficient  |
-30~+70°C |
80 |
+100~+300°C |
93 |
Thermal Conductivity
 |
k |
0.967 |
Mechanical Properties |
Young's Modulus
 |
E |
811 |
Rigidity Modulus
 |
G |
327 |
| Poisson's Ratio |
|
0.240 |
| Knoop Hardness |
Hk |
570 [6] |
| Abrasion |
Aa |
134 |
Photoelastic Constant
 |
|
2.32 |
|
Chemical Properties |
| Water Resistance (P) |
RW(P) |
3 |
| Acid Resistance (P) |
RA(P) |
1 |
| Weathering Resistance (S) |
W(S) |
2~3 |
| Acid Resistance (S) |
SR |
1.0 |
| Phosphate Resistance |
PR |
2.0 |
| P = Powder Group, S = Surface Group |
Other Properties |
| Bubble Quality Group |
B |
1 |
| Specific Gravity |
d |
2.89 |
| Coloring |
|
36 |
|
|
33 |
| |
|
Internal Transmittance |
|
|
|
280 |
|
|
290 |
|
|
300 |
|
|
310 |
|
|
320 |
|
|
330 |
0.090 |
|
340 |
0.440 |
|
350 |
0.740 |
|
360 |
0.880 |
|
365 |
|
|
370 |
0.946 |
|
380 |
0.970 |
|
390 |
0.983 |
|
400 |
0.989 |
|
420 |
0.992 |
|
440 |
0.993 |
|
460 |
0.994 |
|
480 |
0.995 |
|
500 |
0.997 |
|
550 |
0.998 |
|
600 |
0.998 |
|
650 |
0.997 |
|
700 |
0.998 |
|
800 |
0.998 |
|
900 |
0.998 |
|
1000 |
0.997 |
|
1200 |
0.997 |
|
1400 |
0.989 |
|
1600 |
0.993 |
|
1800 |
0.983 |
|
2000 |
0.967 |
|
2200 |
0.914 |
|
2400 |
0.860 |
|
|